Class | ST44-3 (S275J0) |
Number | 10,144 |
Classification | Non-alloy quality structural steel |
Standard | IN 10025-2: 2004 Hot rolled structural steel products. Technical delivery conditions of non-alloy structural steels |
ST44 Chemical Properties of Steel %
C | Mn | P | S | N | With | CEV |
max 0.18 | max 1.5 | max 0.035 | max 0.035 | max 0.012 | max 0.55 | max 0.42 |
Nominal kalınlık = <40 (mm) CEV max = 0.40
ST44 Mechanical Properties of Steel
Nominal thickness (mm): | up to 3 | 3 - 100 | 100 - 150 | 150 - 250 |
Rm - Tensile strength (MPa) Flat and long products | 430-580 | 410-560 | 400-540 | 380-540 |
Nominal thickness (mm): | up to 16 | 16 - 40 | 40 - 63 | 63 - 80 | 80 - 100 | 100 - 150 | 150 - 200 | 200 - 250 |
ReH - Minimum yield power (MPa) Flat and long products | 275 | 265 | 255 | 245 | 235 | 225 | 215 | 205 |
KV - Impact energy (J) longitude, | -20° | 0 ° | + 20 ° | | |
27 | 27 | 27 | | |
| | | | | |
Nominal thickness (mm): | up to 1 | 1 - 1.5 | 1.5 - 2 | 2 - 2,5 | 2,5 - 3 |
A - Min. elongationIt= 80 mm (%) parallel, | 15 | 16 | 17 | 18 | 19 |
| | | | | |
Nominal thickness (mm): | Mar.40 | 40 - 63 | 63 - 100 | 100 - 150 | 150 - 250 |
A - Min. elongationIt= 5.65 √So(%) parallel, | 23 | 22 | 21 | 19 | 18 |
Hot Rolled Non-Alloy Structural Steels
Chemical Composition (%) |
Standard Equivalent | ERDEMIR | C d(thickness, mm) | Mn | P | S | And | With | N(one) | | CE(IIW) (4) max. (%) | |
| | Quality No. | <16 | 16<d<40 | 40<d<100 | | | | | | | | d (mm) | |
Standard | Quality | | max. | max. | max. | max. | max. | max. | max. | max. | max. | <30 | 30<d<40 | 40<d<100 |
IN 10025-2 | S275JR+AR | 3244(5) | 0.21 | 0.21 | 0.22 | 1:50 | 0.035 | 0.035 | - | 0.55 | 0.012 | 0.40 | 0.40 | 0.42 |
Painkllamas
5) For S275 and S355 gradesMax. Carbonandeigenvalue (CEV) for %Si ≤ 0.040.02%, for %Si ≤ 0.250.01% artirritable.